pbayanin tsari
Kamfaninmu yana samar da ingantacciyar ƙarfe-chromium-aluminum da nickel-chromium na walƙiya mai dumama wutar lantarki, waɗanda ke ɗaukar wutar lantarki ta wutar lantarki mai sarrafa kwamfuta kuma an raunata su ta hanyar injin iska mai sauri ta atomatik.Halayen wannan samfurin: babban juriya na zafin jiki, dumama mai sauri, rayuwar sabis na tsawon lokaci, juriya mai ƙarfi, ƙaramin ƙarfin ƙarfi, farar iri ɗaya bayan shimfidawa, farfajiya mai haske da tsabta;Yadu amfani da kananan lantarki tanda, muffle tanderu, dumama da kuma kwandishan kayan aiki, daban-daban tanda, Electric dumama shambura da iyali kayan, da dai sauransu Daban-daban marasa misali masana'antu da farar hula sanduna za a iya tsara da kuma samar bisa ga mai amfani bukatun.
Wutar W | Voltage V | Diamita mm | OD mm | Ltsawo (Reference) mm | Wtakwas g |
300 | 220 | 0.25 | 3.7 | 122 | 1.9 |
500 | 220 | 0.35 | 3.9 | 196 | 4.3 |
600 | 220 | 0.40 | 4.2 | 228 | 6.1 |
800 | 220 | 0.50 | 4.7 | 302 | 11.1 |
1000 | 220 | 0.60 | 4.9 | 407 | 18.5 |
1200 | 220 | 0.70 | 5.6 | 474 | 28.5 |
1500 | 220 | 0.80 | 5.8 | 554 | 39.0 |
2000 | 220 | 0.95 | 6.1 | 676 | 57.9 |
2500 | 220 | 1.10 | 6.9 | 745 | 83.3 |
3000 | 220 | 1.20 | 7.1 | 792 | 98.3 |
Yanayin zafin jiki da sinadaran sinadaran na wayar dumama
Daraja | Max.Ci gaba Tsananin Aiki. | Cr% | Ni% | Al% | Fe% | Re% | Nb% | Mo% |
Cr20Ni80 | 1200 ℃ | 20-23 | Bal. |
|
|
|
|
|
Cr30Ni70 | 1250 ℃ | 28-31 | Bal. |
|
|
|
|
|
Cr15Ni60 | 1150 ℃ | 15-18 | 55 zuwa 61 |
| Bal. |
|
|
|
Cr20Ni35 | 1100 ℃ | 18-21 | 34 zuwa 37 |
| Bal. |
|
|
|
TANKI APM | 1425 ℃ | 20.5 ~ 23.5 |
| 5.8 | Bal. | / |
|
|
0Cr27Al7Mo2 | 1400 ℃ | 26.5-27.8 |
| 6 ~ 7 | Bal. |
|
| 2 |
0Cr21Al6Nb | 1350 ℃ | 21-23 |
| 5 ~ 7 | Bal. |
| 0.5 |
|
0Cr25Al5 | 1250 ℃ | 23 ~ 26 |
| 4.5 ~ 6.5 | Bal. |
|
|
|
0Cr23Al5Y | 1300 ℃ | 22.5 ~ 24.5 |
| 4.2 ~ 5.0 | Bal. |
|
|
|
0Cr19Al3 | 1100 ℃ | 18-21 |
| 3 ~ 4.2 | Bal. |
|
|
|
Babban kayan fasaha na FeCrAl alloy waya:
①A amfani zafin jiki ne high, da amfani zafin jiki na baƙin ƙarfe-chromium aluminum gami waya a cikin yanayi iya isa 1300 ℃;
② Rayuwa mai tsawo;
③Abin da aka yarda da shi yana da girma;
⑤Takamammen nauyi ya fi ƙarami fiye da gami da nickel-chromium;④ Rashin haɓakar iskar oxygen yana da kyau, kuma fim din AI2O3 da aka kafa bayan oxidation yana da kyakkyawan juriya na sinadarai da kuma tsayayyar haɓaka;
⑥ High resistivity;
⑦ Kyakkyawan juriya na sulfur;
⑧Farashin yana da mahimmanci ƙasa da na nickel-chromium gami;
⑨Rashin lahani shine yayin da zafin jiki ya karu, yana nuna filastik, kuma ƙarfin a yanayin zafi yana da ƙasa.
Halayen wayar murhu na nickel-chromium sune:
① Babban ƙarfi a babban zafin jiki;
② kwantar da hankali bayan amfani da dogon lokaci, kayan ba zai zama gagara ba;
③Sakamakon iskar oxidized Ni-ming gami ya fi na Fe-Cr-Al alloy;
④ Babu maganadisu;
⑤ Ban da yanayin sulfur, yana da mafi kyawun juriya na lalata