Tare da ƙananan ƙididdiga masu zafi na juriya na lantarki, juriya, don haka aiki, yana da daidaituwa ba tare da la'akari da zafin jiki ba. Copper Nickel Alloys na inji suna alfahari mai kyau ductility, ana iya siyar da su cikin sauƙi da waldi, kuma suna da juriya na lalata. Ana amfani da waɗannan gami a cikin manyan aikace-aikacen yanzu waɗanda ke buƙatar babban matakin daidaici.


  • Daraja:KuNi44
  • Girman:0.16mm
  • Girma (g/cm³):8.9
  • Tsawaita(%):≥25
  • Matsakaicin zafin aiki (uΩ/m a 20°C):0.49
  • Launi:Mai haske
  • Cikakken Bayani

    FAQ

    Tags samfurin

    Alloys na nickel (CuNi) matsakaici ne zuwa ƙananan kayan juriya yawanci ana amfani da su a aikace-aikace tare da matsakaicin yanayin aiki har zuwa 400°C (750°F).
    Tare da ƙananan ƙididdiga masu zafi na juriya na lantarki, juriya, don haka aiki, yana da daidaituwa ba tare da la'akari da zafin jiki ba. Copper Nickel Alloys na inji suna alfahari mai kyau ductility, ana iya siyar da su cikin sauƙi da waldi, kuma suna da juriya na lalata. Ana amfani da waɗannan gami a cikin manyan aikace-aikacen yanzu waɗanda ke buƙatar babban matakin daidaici.

    Daraja KuNi44 KuNi23 KuNi10 KuNi6 KuNi2 KuNi1 KuNi8 KuNi14 KuNi19 KuNi30 KuNi34 KuMn3
    Cuprothal 49 30 15 10 5
    Isabellehutte ISOTAN Alloy 180 Allo 90 Alloy 60 Alloy 30 ISA 13
    Abun ƙima% Ni 44 23 10 6 2 1 8 14 19 30 34 -
    Cu Bal Bal Bal. Bal. Bal. Bal. Bal. Bal. Bal Bal Bal Bal
    Mn 1 0.5 0.3 - - - - 0.5 0.5 1.0 1.0 3.0
    Matsakaicin zafin aiki (uΩ/m a 20°C) 0.49 0.3 0.15 0.10 0.05 0.03 0.12 0.20 0.25 0.35 0.4 0.12
    Resisivity (Ω/cmf a 68°F) 295 180 90 60 30 15 72 120 150 210 240 72
    Matsakaicin zafin aiki (°C) 400 300 250 200 200 200 250 300 300 350 350 200
    Girma (g/cm³) 8.9 8.9 8.9 8.9 8.9 8.9 8.9 8.9 8.9 8.9 8.9 8.9
    TCR(×10-6/°C) <-6 <16 <50 <60 <120 <100 <57 <30 <25 <10 <0 <38
    Ƙarfin Tensile (Mpa) ≥420 ≥350 ≥290 ≥250 ≥220 ≥210 ≥270 ≥310 ≥340 ≥400 ≥400 ≥290
    Tsawaita(%) ≥25 ≥25 ≥25 ≥25 ≥25 ≥25 ≥25 ≥25 ≥25 ≥25 ≥25 ≥25
    EMF vs Cu uV/°C (0 ~ 100°C) -43 -34 -25 -12 -12 -8 22 -28 -32 -37 -39 -
    Wurin narkewa (°C) 1280 1150 1100 1095 1090 1085 1097 1115 1135 1170 1180 1050
    Abubuwan Magnetic ba ba ba ba ba ba ba ba ba ba ba ba